 +Deposition date: 20060406
 +
 +Target: Pr0.5Ca0.5MO3 compound target \\
 +Substrate: STO-Nb \\
 +Pressure: 3 mbar O2 \\
 +Flow: 40 ml/min \\
 +Current: 200 mA \\
 +Voltage: 418 V \\
 +Time: 150 min \\
 +Temp: 840 C \\
 +Remarks: -\\
 +----
 +XRR: \\
 +Result: 160 nm\\
 +----
 +RBS: \\
 +Run: 20060512 \\
 +File: pr83 \\
 +Result: Channeling! peak supression in substrate much stronger than in film = > not (fully) epitaxial. Measurement repeated with tilt and rotation. Fit values see pr83_tilt3_rot3. \\
 +Postscript: {{sdb:pr83.ps}}
 +----
 +RBS: \\
 +Run: 20060512 \\
 +File: pr83_tilt3_rot3 \\
 +Result: 60 nm Pr .07 Ca .07 Mn 0.1 O .75 (sens. for O is low, O conc. is entangled with density) \\
 +Postscript: {{sdb:pr83_tilt3_rot3.ps}}
 +
  